Sandvik 3R64 is an austenitic stainless steel with a high molybdenum content. The grade is characterized by improved resistance to general and pitting corrosion in comparison with ASTM 316L.
Standards
-
: TP317L -
: S31703 -
: 2367
Product standards
Seamless tube and pipe
ASTM A213, A312
SS 142367
Chemical composition (nominal)
C | Si | Mn | P | S | Cr | Ni | Mo |
---|---|---|---|---|---|---|---|
≤0.030 | 0.4 | 1.7 | ≤0.030 | ≤0.015 | 18.5 | 14.5 | 3.1 |
Applications
Sandvik 3R64 can be used for a wide range of industrial applications where steels of type ASTM 304 and 304L or even ASTM 316L have insufficient corrosion resistance. Typical examples are heat exchangers, condensers, pipelines, cooling and heating coils in the chemical, petrochemical, pulp and paper and food industries.
Corrosion resistance
Owing to its high molybdenum content Sandvik 3R64 possesses improved resistance compared to ASTM 316/316L in a majority of chloride and acidic environments.
General corrosion
Sandvik 3R64 has good resistance in:
- Organic acids at high concentrations and moderate temperatures
- Inorganic acids, e.g. phosphoric and sulphuric acids at moderate concentrations and temperatures. The steel can also be used in sulphuric acid of concentrations above 90% at low temperature
- Salt solutions, e.g. sulphates, sulphides and sulphites caustic environments
The following data illustrate the improved resistance of Sandvik 3R64 vs ASTM 316, although the corrosion rates at the majority of temperatures are unacceptably high for both grades.
Table 1. General corrosion resistance of Sandvik 3R64 and ASTM 316 in boiling formic acid.
Formic acid, wt-%
|
Corrosion rate, mm/year
|
|
---|---|---|
Sandvik 3R64 | ASTM 316 | |
5 | 0.12 | 0.18 |
10 | 0.20 | 0.3 |
25 | 0.35 | 0.6 |
50 | 0.45 | 0.6 |
80 | 1.0 | 1.5 |
90 | 0.8 | 1.8 |
100
|
0.4
|
0.6
|
Intergranular corrosion
Owing to its low carbon content Sandvik 3R64 possesses a low risk for intergranular corrosion after e.g. welding operations.
Pitting and crevice corrosion
The pitting corrosion resistance of stainless steels is primarily determined by the contents chromium, molybdenum and nitrogen. The Pitting Resistance Equivalent can be used for ranking different stainless steels with regard to their pitting resistance. The PRE number is defined as:
PRE = % Cr + 3.3 x % Mo + 16 x % N
Table 2. PRE values for Sandvik 3R64 and some other alloys. Typical values unless otherwise stated
Alloy | 3R64 | ASTM 316L1) | Alloy 825 | 904L | SAF 2205 |
---|---|---|---|---|---|
PRE | 29 | 24 | 31 | 34 | >35 |
1) 2.1 % Mo
Thus Sandvik 3R64 is resistant against pitting corrosion at higher temperatures and/or higher chloride concentrations than is the case for ASTM 316L.
Figure 1. Crevice corrosion resistance of Sandvik 3R64 and 3R60.
The same ranking of alloys can be applied for the crevice corrosion resistance. However, crevice corrosion is to be expected at significantly lower temperatures, than is the case for pitting corrosion. Figure 1 demonstrates the better crevice corrosion resistance of Sandvik 3R64 vs. 3R60 (ASTM 316L with 2.6% Mo, EN 1.4435) after 2 months exposure in chloride solutions.
Stress corrosion cracking
Austenitic steels are susceptible to stress corrosion cracking. This may occur at temperatures above about 60°C (140°F) if the steel is subjected to tensile stresses and at the same time comes into contact with certain solutions, particularly those containing chlorides. Such service conditions should therefore be avoided. Conditions when plants are shut down must also be considered, as the condensates which are then formed can develop a chloride content that leads to both stress corrosion cracking and pitting.
In applications demanding high resistance to stress corrosion cracking, austenitic-ferritic steels, such as Sandvik SAF 2304 or Sandvik SAF 2205 are recommended. See data sheets S-1871-ENG or S-1874-ENG.
Forms of supply
Seamless tube and pipe
Seamless tube and pipe in 3R64 is supplied in dimensions up to 260 mm outside diameter in the solution annealed and white-pickled condition or solution annealed in a bright-annealing process.
Other forms of supply
Sandvik 3R64 is also supplied in forms of:
- Welded tube and pipe
- Fittings and flanges
Further details concerning sizes and finishes are available on request.
Heat treatment
The tubes are delivered in heat treated condition. If additional heat treatment is needed after further processing the following is recommended.
Stress relieving
850–950°C (1560–1740°F), 10-15 min, cooling in air.
Solution annealing
1000–1100°C (1830–2010°F), 10-30 min, cooling in air or water.
Mechanical properties
For tube and pipe with a wall thickness greater than 10 mm (0.4 in.) the proof strength may fall short of the stated values by about 10 MPa (1.4 ksi).
At 20°C (68°F)
Proof strength | Tensile strength | Elong. | Hardness | |
---|---|---|---|---|
Rp0.2a | Rp1.0a | Rm | Ab | Vickers |
MPa | MPa | MPa | % | |
approx. | ||||
≥220 | ≥250 | 515-690 | ≥35 | 155 |
Proof strength | Tensile strength | Elong. | Hardness | |
---|---|---|---|---|
Rp0.2a | Rp1.0a | Rm | Ab | Vickers |
ksi | ksi | ksi | % | |
approx. | ||||
≥32 | ≥36 | 75-100 | ≥35 | 155 |
1 MPa = 1 N/mm2
a) Rp0.2 and Rp1.0 correspond to 0.2% offset and 1.0% offset yield strength, respectively.
b) Based on L0 = 5.65 ÖS0 where L0 is the original gauge length and S0 the original cross-section area.
Impact strength
Due to its austenitic microstructure, Sandvik 3R64 has very good impact strength both at room temperature and at cryogenic temperatures.
Tests have demonstrated that the steel fulfils the requirements according to the European standards EN 13445-2 (UFPV-2) ( (min. 60 J (44 ft-lb) at -270 oC (-455 oF)) and EN 10216-5 (min. 60 J (44 ft-lb) at -196 oC (-320oF).
At high temperatures
Temperature | Proof strength | |
---|---|---|
°C | Rp0.2a | Rp1.0a |
MPa | MPa | |
min. | min. | |
50 | 196 | 221 |
100 | 172 | 197 |
150 | 155 | 180 |
200 | 144 | 169 |
250 | 136 | 161 |
300 | 129 | 154 |
350 | 123 | 148 |
400 | 119 | 144 |
450 | 115 | 140 |
500 | 110 | 135 |
Temperature | Proof strength | |
---|---|---|
°F | Rp0.2a | Rp1.0a |
MPa | ksi | |
min. | min. | |
200 | 25.4 | 29.0 |
400 | 20.8 | 24.4 |
600 | 18.4 | 22.1 |
800 | 17.0 | 20.6 |
1000 | 15.4 | 19.0 |
Physical properties
Density: 8.0 g/cm3, 0.29 lb/in3
Temperature, °C | W/m °C | Temperature, °F | Btu/ft h °F |
---|---|---|---|
20 | 14 | 68 | 8 |
100 | 15 | 200 | 8.5 |
200 | 17 | 400 | 10 |
300 | 18 | 600 | 10.5 |
400 | 20 | 800 | 11.5 |
500 | 21 | 1000 | 12.5 |
600 | 23 | 1100 | 13 |
Temperature, °C | J/kg °C | Temperature, °F | Btu/lb °F |
---|---|---|---|
20 | 485 | 68 | 0.11 |
100 | 500 | 200 | 0.12 |
200 | 515 | 400 | 0.12 |
300 | 525 | 600 | 0.13 |
400 | 540 | 800 | 0.13 |
500 | 555 | 1000 | 0.13 |
600 | 575 | 1100 | 0.14 |
Temperature, °C | Per °C | Temperature, °F | Per °F |
---|---|---|---|
30-100 | 16.5 | 86-200 | 9.5 |
30-200 | 17 | 86-400 | 9.5 |
30-300 | 17.5 | 86-600 | 10 |
30-400 | 18 | 86-800 | 10 |
30-500 | 18 | 86-1000 | 10 |
30-600 | 18 | 86-1200 | 10.5 |
30-700 | 18.5 | 86-1400 | 10.5 |
1) Mean values in temperature ranges (x10-6)
Temperature, °C | MPa | Temperature, °F | ksi |
---|---|---|---|
20 | 200 | 68 | 29.0 |
100 | 194 | 200 | 28.2 |
200 | 186 | 400 | 26.9 |
300 | 179 | 600 | 25.8 |
400 | 172 | 800 | 24.7 |
500 | 165 | 1000 | 23.5 |
1) (X103)
Welding
The weldability of Sandvik 3R64 is good. Welding must be carried out without preheating and subsequent heat treatment is normally not required. Suitable methods of fusion welding are manual metal-arc welding (MMA/SMAW) and gas-shielded arc welding, with the TIG/GTAW method as first choice.
For Sandvik 3R64, heat input of <1.5 kJ/mm and interpass temperature of <100°C (210°F) are recommended.
Recommended filler metals
TIG/GTAW or MIG/GMAW welding
ISO 14343 S 19 13 4 L / AWS A5.9 ER317L (e.g. Exaton 19.13.4.L)
MMA/SMAW welding
ISO 3581 E 19 13 4 L R / AWS A5.4 E317L-16 (e.g. Exaton 19.13.4.LR)
ISO 14343 S 19 13 4 L / AWS A5.9 ER317L (e.g. Exaton 19.13.4.L) wire or strip electrodes are recommended for overlay welding of tube sheets and high-pressure vessels in cases where corrosion resistance, equal to that of Sandvik 3R64, is required.