These corrosion data are mainly based on results of general corrosion laboratory tests, carried out with pure chemicals and water solutions nearly saturated with air (the corrosion rate can be quite different if the solution is free from oxygen).

All concentrations are given in weight-% and the solvent is water if nothing else is shown. The corrosion data apply to annealed materials with normal microstructure and clean surfaces, throughout.

Chlorine, Cl2
Conc. Cl2abbcda) dry gas 100% b) moist gas c) Aqueous soln 1 mg/l d) Aqueous soln 1g/l
Temp. °C7020-6060-1002020
Grade or type of alloy:
Carbon steel0221p
13 Cr0220p
Alleima® 18020220
Alleima® 3R1202201p
Alleima® 3R6002201p
18Cr13Ni3Mo 1)
02201p
17Cr14Ni4Mo 2)
02200p
Alleima® 2RK65 ('904L')01p200p
Sanicro® 28
254 SMO2
654 SMO1ND
SAF™ 2304
SAF™ 22052
SAF™ 25072
Titanium (CP Ti)20000

1) ASTM 317L, e.g. Alleima® 3R64
2) EN 1.4439, e.g. Alleima® 3R68

Symbol clarification

These corrosion tables use a number of symbols, having the following meanings:

Symbol Description
0 Corrosion rate less than 0.1 mm/year. The material is corrosion proof.
1 Corrosion rate 0.1—1.0 mm/year. The material is not corrosion proof, but useful in certain cases.
2 Corrosion rate over 1.0 mm/year. Serious corrosion. The material is not usable.
p, P Risk (severe risk) of pitting and crevice corrosion.
c, C Risk (Severe risk) of crevice corrosion. Used when there is a risk of localised corrosion only if crevices are present. Under more severe conditions, when there is also a risk of pitting corrosion, the symbols p or P are used instead.
s, S Risk (Severe risk) of stress corrosion cracking.
ig Risk of intergranular corrosion.
BP Boiling solution.
ND No data. (Used only where there are no actual data to estimate the risk of localised corrosion instead of p or s).

Disclaimer: Laboratory tests are not strictly comparable with actual service conditions. Accordingly, Alleima makes no warranties, express or implied, and accept no liability, compensatory or consequential, for the performance of different materials in individual applications that may be based on the information provided in this publication.