2024-01-11 10:29
(supersedes all previous editions)
Sanmac® 4305 is an austenitic chromium-nickel steel with extremely high machinability. For example, cutting speeds of up to twice those for Sanmac 304/304L can be used.
C |
Si | Mn | P |
S | Cr | Ni |
---|---|---|---|---|---|---|
≤0.035 | 0.4 | 1.8 | ≤0.040 | 0.2 | 17.5 | 9 |
Sanmac® 4305 is a good choice for components where high machinability is needed, but where corrosion resistance and high stresses are not a concern.
Sanmac® 4305 has good resistance to:
Sanmac® 4305 has a low carbon content and therefore good resistance to intergranular corrosion.
Austenitic steels are susceptible to stress corrosion cracking. This may occur at temperatures above about 60°C (140°F) if the steel is subjected to tensile stresses and at the same time comes into contact with certain solutions, particularly those containing chlorides. In applications demanding high resistance to stress corrosion cracking the austenitic-ferritic steels SAF 2304®, Alleima® 10RE51 or Sanmac® 2205 have higher resistance to stress corrosion cracking than 4305.
The steel may be sensitive to pitting and crevice corrosion even in solutions of relatively low chloride content. Molybdenum-alloyed steels have better resistance and the resistance improves with increasing molybdenum content.
Hollow bar- Finishes, dimensions and tolerances
Hollow bar in Sanmac® 4305 can be produced in various sizes in the solution annealed and white-pickled condition.
Dimensions are given as outside and inside diameters with guaranteed component sizes after machining, see catalogues.
Outside diameter tolerance is +2/-0%, but minimum +1/-0mm
Inside diameter tolerance is +0/-2%, but minimum +0/-1mm
Straightness +/-1.5mm/m
Better tolerances can be supplied on special order.
Other forms of supply
Bar
Steel with improved machinability, Sanmac, is also available in bar.
Hollow bar is delivered in heat treated condition. If further heat treatment is needed after further processing the following is recommended:
Stress relieving
850–950°C (1560–1740°F), cooling in air.
Solution annealing
1000–1100°C (1830–2010°F), rapid cooling in air or water.
Proof strength | Tensile strength | Elong. | Hardness | ||
---|---|---|---|---|---|
Rp0.2a | Rp1.0a | Rm | Ab | A2" | HRB |
MPa | MPa | MPa | % | % | |
≥210 | ≥230 | ≥515 | ≥35 | ≥35 | ≤90 |
Proof strength | Tensile strength | Elong. | Hardness | ||
---|---|---|---|---|---|
Rp0.2a | Rp1.0a | Rm | Ab | A2" | HRB |
ksi | ksi | ksi | % | % | |
≥30 | ≥33 | ≥75 | ≥35 | ≥35 | ≤90 |
1 MPa = 1N/mm2
a)Rp0.2 and Rp1.0 correspond to 0.2% offset and 1.0% offset yield strength, respectively.
b) Based on L0 = 5.65 ÖS0 where L0 is the original gauge length and S0 the original cross-section area.
Sanmac® 4305 possesses good impact strength both at room temperature and at low temperatures.
Density: 7.9 g/cm3, 0.29 lb/in3
Temperature, °C | W/m °C | Temperature, °F | Btu/ft h °F |
---|---|---|---|
20 | 15 | 68 | 8.5 |
100 | 16 | 200 | 9.5 |
200 | 18 | 400 | 19.5 |
300 | 20 | 600 | 12 |
400 | 22 | 800 | 13 |
500 | 23 | 1000 | 14 |
600 | 25 | 1200 | 15 |
700 | 26 | 1300 | 15 |
Temperature, °C | J/kg °C | Temperature, °F | Btu/lb °F |
---|---|---|---|
20 | 475 | 68 | 0.11 |
100 | 500 | 200 | 0.12 |
200 | 530 | 400 | 0.13 |
300 | 560 | 600 | 0.13 |
400 | 580 | 800 | 0.14 |
500 | 600 | 1000 | 0.14 |
600 | 615 | 1200 | 0.15 |
700 | 625 | 1300 | 0.15 |
Temperature, °C | Per °C | Temperature, °F | Per °F |
---|---|---|---|
30-100 | 16.5 | 86-200 | 9.5 |
30-200 | 17 | 86-400 | 9.5 |
30-300 | 17.5 | 86-600 | 10 |
30-400 | 18 | 86-800 | 10 |
30-500 | 18.5 | 86-1000 | 10 |
30-600 | 18.5 | 86-1200 | 10.5 |
30-700 | 19 | 86-1400 | 10.5 |
Temperature, °C | MPa | Temperature, °F | ksi |
---|---|---|---|
20 | 200 | 68 | 29.0 |
100 | 194 | 200 | 28.2 |
200 | 186 | 400 | 26.9 |
300 | 179 | 600 | 25.8 |
400 | 172 | 800 | 24.7 |
500 | 165 | 1000 | 23.5 |
Welding of Sanmac® 4305 should be carried out with filler material under carefully control due to Sulphur addition in the material. Suitable methods of fusion welding are manual metal-arc welding (MMA/SMAW) and gas-shielded arc welding, with the TIG/GTAW method as first choice.
For Sanmac® 4305, heat input of <1.0 kJ/mm and interpass temperature of <100°C (210°F) are recommended.
TIG/GTAW or MIG/GMAW welding
ISO 14343 S 19 9 L / AWS A5.9 ER308L (e.g. Exaton 19.9.L)
ISO 14343 S 23 12 L / AWS A5.9 ER309L (e.g. Exaton 24.13.L)
ISO 14343 S 18 8 Mn / AWS A5.9 ER307 (e.g. Exaton 18.8.Mn)
MMA/SMAW welding
ISO 3581 E 19 9 L R / AWS A5.4 E308L-17(e.g. Exaton 19.9.LR)
ISO 3581 E 23 12 L R / AWS A5.4 E309L-17(e.g. Exaton 24.13.LR)
Sanmac is our trademark for the Alleima machinability concept. In SANMAC materials, machinability has been improved without jeopardising properties such as corrosion resistance and mechanical strength.
The improved machinability is owing to:
Detailed recommendations for the choice of tools and cutting data regarding turning, thread cutting, parting/grooving, drilling, milling and sawing are provided in the brochure S-02909-ENG.
The diagram shows the ranges within which data should be chosen in order to obtain a tool life of minimum 10 minutes when machining austenitic SANMAC materials (304/304L, 316/316L).
[bild]
The ranges are limited in the event of low feeds because of unacceptable chip breaking. In the case of high cutting speeds, plastic deformation is the most dominant cause of failure. When feed increases and the cutting speed falls, edge frittering (chipping) increases significantly. The diagram is applicable for short cutting times. For long, continuous cuts, the cutting speeds should be reduced somewhat.
The lowest recommended cutting speed is determined by the tendency of the material to stick to the insert (built-up-edge), although the integrity of insert clamping and the stability of the machine are also of great significance.
It is important to conclude which wear mechanism is active, in order to optimise cutting data with the aid of the diagram.
Disclaimer: Recommendations are for guidance only, and the suitability of a material for a specific application can be confirmed only when we know the actual service conditions. Continuous development may necessitate changes in technical data without notice. This datasheet is only valid for Alleima materials.