These corrosion data are mainly based on results of general corrosion laboratory tests, carried out with pure chemicals and water solutions nearly saturated with air (the corrosion rate can be quite different if the solution is free from oxygen).

All concentrations are given in weight-% and the solvent is water if nothing else is shown. The corrosion data apply to annealed materials with normal microstructure and clean surfaces, throughout.

Chromium trioxide, chromic acid, CrO3
Conc. CrO3%22551010202020404050
Temp. °C75100=BP80100=BP40BP2050BP204020
Grade or type of alloy:
Carbon steel2202022011
13 Cr22022222
Alleima® 180222021222
Alleima® 3R12020102012122
Alleima® 3R60020202012122
18Cr13Ni3Mo 1)
02020201222
17Cr14Ni4Mo 2)
0212021222
Alleima® 2RK65 ('904L')02010201222
Sanicro® 2800010212122
254 SMO00010212122
654 SMO
SAF™ 230400010212122
SAF™ 220500120222222
SAF™ 250700120222222
Titanium (CP Ti)000000000000

1) ASTM 317L, e.g. Alleima® 3R64
2) EN 1.4439, e.g. Alleima® 3R68

Symbol clarification

These corrosion tables use a number of symbols, having the following meanings:

Symbol Description
0 Corrosion rate less than 0.1 mm/year. The material is corrosion proof.
1 Corrosion rate 0.1—1.0 mm/year. The material is not corrosion proof, but useful in certain cases.
2 Corrosion rate over 1.0 mm/year. Serious corrosion. The material is not usable.
p, P Risk (severe risk) of pitting and crevice corrosion.
c, C Risk (Severe risk) of crevice corrosion. Used when there is a risk of localised corrosion only if crevices are present. Under more severe conditions, when there is also a risk of pitting corrosion, the symbols p or P are used instead.
s, S Risk (Severe risk) of stress corrosion cracking.
ig Risk of intergranular corrosion.
BP Boiling solution.
ND No data. (Used only where there are no actual data to estimate the risk of localised corrosion instead of p or s).

Disclaimer: Laboratory tests are not strictly comparable with actual service conditions. Accordingly, Alleima makes no warranties, express or implied, and accept no liability, compensatory or consequential, for the performance of different materials in individual applications that may be based on the information provided in this publication.