Tube, pipe, fittings and flanges
Control lines and chemical injection lines in austenitic stainless steel and duplex stainless steel. Our range includes control lines and chemical injection lines in seamless or welded condition.
Alleima offers a quick and effective solution whether the order is for straightforward, cut to length lines or a group of lines, encapsulated, flushed and filled, supplied on customer's own reels and delivered direct to site.
Alleima also provides coiled tubing for umbilicals.
Alleima's service center in Houston (TX), US holds extensive seamless coiled tube and laser welded tube stocks for control lines and chemical injection lines to ensure just-in-time deliveries. It also operates a complete package of additional services:
The tables show materials, sizes and approvals for control lines and chemical injection lines in seamless condition.
Grade | UNS | C max. | Cr | Ni | Mo | N | Others |
---|---|---|---|---|---|---|---|
TP 316L | S31600/S31603 | 0.030 | 17.5 | 13 | 2.1 | - | - |
Alloy 825 | N08825 | 0.030 | 20 | 38.5 | 2.6 | - | Cu=1.7, Ti=0.7 |
Sanicro® 28 | N08028 | 0.020 | 27 | 31 | 3.5 | - | Cu=1.0 |
Alleima SAF 2205™ | S31803/S32205 | 0.030 | 22 | 5 | 3.2 | 0.18 | - |
Alleima SAF 2507® | S32750 | 0.030 | 25 | 7 | 4 | 0.3 | - |
* All materials are supplied in the solution annealed condition. Other grades can be offered on request.
Grade | Yield strength, psi (MPa) |
Tensile strength, psi (MPa) |
Elongation % |
---|---|---|---|
TP 316L | 32,000 (220) | 75,000 (515) | 35 |
Alloy 825 | 35,000 (240) | 80,000 (550) | 30 |
Sanicro® 28 | 32,000 (220) | 100,000 (690) | 40 |
Alleima SAF 2205™ | 70,000 (485) | 99,000 (680) | 25 |
Alleima SAF 2507® | 80,000 (550) | 116,000 (800) | 25 |
1) All materials in the solution annealed condition
Grade | UNS | PRE1) | CPT2) o F (oC) |
Max. H2S3 psi | CO24) |
---|---|---|---|---|---|
TP 316L | S31600/S31603 | 24 | 95 (35) | No Limit | + |
Alloy 825 | N08825 | 29 | 140 (60) | No Limit | ++ |
Sanicro® 28 | N08028 | 39 | 150 (65) | No Limit | ++ |
Alleima SAF 2205™ | S31803/S32205 | >35 | 150 (65) | 1.5 | + |
Alleima SAF 2507® | S32750 | >42.5 | 195 (90) | 3 | ++ |
1) PRE = (%Cr) + 3.3 (%Mo) +16 (%N)
2) Critical Pitting Temperature in neutral solution with approximately 3% chlorides
3) Per NACE MR0175 / ISO 15156 for downhole control lines in the solution annealed condition
4) General resistance to CO2 corrosion. '++' indicates better resistance than '+'
Outside diameter | Wall thickness | Max single coil length (TP 316L) | Max single coil length (A825) |
Max LLBW1) 2) | |||
---|---|---|---|---|---|---|---|
in. | in. | m | ft | m | ft | m | ft |
1/4 | 0.035 | 252 | 827 | 640 | 2,100 | 29,000 | 95,149 |
1/4 | 0.049 | 192 | 630 | 488 | 1,601 | 22,000 | 72,182 |
1/4 | 0.065 | 158 | 518 | 401 | 1,316 | 18,000 | 59,058 |
3/8 | 0.035 | 159 | 522 | 404 | 1,326 | 18,000 | 59,058 |
3/8 | 0.049 | 118 | 387 | 300 | 984 | 14,000 | 45,934 |
3/8 | 0.065 | 94 | 308 | 239 | 784 | 11,000 | 36,091 |
3/8 | 0.083 | 78 | 256 | 199 | 653 | 9,000 | 29,529 |
1/2 | 0.035 | 116 | 381 | 296 | 971 | 13,000 | 24,653 |
1/2 | 0.049 | 85 | 279 | 217 | 712 | 10,000 | 32,810 |
1/2 | 0.065 | 67 | 220 | 171 | 561 | 7,500 | 24,608 |
1/2 | 0.083 | 55 | 180 | 139 | 456 | 6,000 | 19,686 |
5/8 | 0.035 | 92 | 302 | 234 | 767 | 10,750 | 35,271 |
5/8 | 0.049 | 67 | 220 | 171 | 561 | 7,500 | 24,608 |
5/8 | 0.065 | 52 | 171 | 131 | 430 | 6,100 | 20,014 |
5/8 | 0.083 | 25 | 82 | 25 | 82 | 5,000 | 16,405 |
3/4 | 0.035 | 25 | 82 | 25 | 82 | - | - |
3/4 | 0.049 | 25 | 82 | 25 | 82 | - | - |
3/4 | 0.065 | 25 | 82 | 25 | 82 | - | - |
3/4 | 0.083 | 25 | 82 | 25 | 82 | - | - |
1) Long length butt welded
2) For 3/4 in. OD single coils can be made. Contact us for complete details.
The tables show materials, sizes and approvals for control lines and chemical injection lines in welded condition.
Grade | UNS | C max. |
Cr | Ni | Mo | Others |
---|---|---|---|---|---|---|
TP 316L | S31600/S31603 | 0.030 | 17.5 | 13 | 2.1 | 0.1 |
Alloy 825 | N08825 | 0.030 | 20 | 38.5 | 2.6 | Cu=1.7, Ti=0.7 |
Alloy 625 | N6625 | 0.10 | 21.5 | >=58 | 9 | Nb=3.5 |
*All materials are supplied in the solution annealed condition. Other grades can be offered on request.
Grade | Yield strength, psi (MPa) |
Tensile strength, psi (MPa) |
Elongation % |
---|---|---|---|
TP 316L | 32,000 (220) | 75,000 (515) | 35 |
Alloy 825 | 35,000 (240) | 80,000 (550) | 30 |
Alloy 625 | 60,000 (415) | 110,000 (760) | 30 |
1) All materials in the solution annealed condition
Grade | UNS | PRE1) | CPT2) F (oC) | Max H2S3) psi | CO24) |
---|---|---|---|---|---|
TP 316L | S31600/S31603 | 24 | 95 (35) | No limit | + |
Alloy 825 | N08825 | 29 | 140 (60) | No limit | ++ |
Alloy 625 | N06625 | 52 | 195 (90) | No limit | ++ |
1) PRE = (%Cr) + 3.3 (%Mo) +16 (%N)
2) Critical Pitting Temperature in neutral solution with approximately 3% chlorides
3) Per NACE MR0175 / ISO 15156 for downhole control lines in the solution annealed condition
4) General resistance to CO2 corrosion. '++' indicates better resistance than '+'
The table shows stock standard sizes. Other sizes can be offered on request.
OD | WT | OD | WT | OD | WT | OD | WT | OD | WT |
---|---|---|---|---|---|---|---|---|---|
1/4 | 0.035 | 3/8 | 0.035 | 1/2 | 0.035 | 5/8 | 0.035 | 3/4 | 0.035 |
1/4 | 0.049 | 3/8 | 0.049 | 1/2 | 0.049 | 5/8 | 0.049 | 3/4 | 0.049 |
1/4 | 0.065 | 3/8 | 0.065 | 1/2 | 0.065 | 5/8 | 0.065 | 3/4 | 0.065 |
- | - | 3/8 | 0.083 | 1/2 | 0.083 | 5/8 | 0.083 | 3/4 | 0.083 |
OD = Outside diameter, WT = Wall thickness
Alleima offers a wide range of encapsulation materials. The most frequent ones can be found in the table below. Other encapsulation materials can be offered upon request.
Material rating on a scale of 1 to 5 (1=not good, 5=excellent)
Materials | Max temp. oF (Co) |
Abrasion resistance | Resistance to inhibited brine well fluids | Resistance to oil/diesel well fluids |
---|---|---|---|---|
Polypropylene | 150 (65) | 2 | 5 | 3 |
Nylon 11 | 200 (93) | 4 | 3 | 3 |
PVC | 174 (79) | 3 | 2 | 3 |
TPV | 275 (135) | 3 | 5 | 3 |
Halar | 300 (149) | 4 | 4 | 5 |
PVDF | 310 (154) | 4 | 3 | 5 |
MPH340G | 340 /171) | 4 | 4 | 5 |
Selection of the appropriate material for any given control or chemical injection line is subject to the prevailing operational and site conditions. In order to assist in the selection, the following tables provide internal pressure ratings and the adjustments factors for a range of common grades and sizes of seamless and laser welded stainless tubing.
Please refer to grade and product form adjustment factors below.
Outside diameter, in. | Wall thickness, in. | Working pressure2) psi (MPa) |
Burst pressure2) psi (MPa) |
Collapse pressure4) psi (MPa) |
---|---|---|---|---|
1/4 | 0.035 | 6,600 (46) | 22,470 (155) | 6,600 (46) |
1/4 | 0.049 | 9,260 (64) | 27,400 (189) | 8,710 (60) |
1/4 | 0.065 | 12,280 (85) | 34,640 (239) | 10,750 (74) |
3/8 | 0.035 | 4,410 (30) | 19,160 (132) | 4,610 (32) |
3/8 | 0.049 | 6,170 (43) | 21,750 (150) | 6,220 (43) |
3/8 | 0.065 | 8,190 (56) | 25,260 (174) | 7,900 (54) |
3/8 | 0.083 | 10,450 (72) | 30,050 (207) | 9,570 (66) |
1/2 | 0.049 | 4,630 (32) | 19,460 (134) | 4,820 (33) |
1/2 | 0.065 | 6,140 (42) | 21,700 (150) | 6,200 (43) |
1/2 | 0.083 | 7,840 (54) | 24,600 (170) | 7,620 (53) |
5/8 | 0.049 | 3,700 (26) | 18,230 (126) | 3,930 (27) |
5/8 | 0.065 | 4,900 (34) | 19,860 (137) | 5,090 (35) |
5/8 | 0.083 | 6,270 (43) | 26,910 (151) | 6,310 (44) |
3/4 | 0.049 | 3,080 (21) | 17,470 (120) | 3,320 (23) |
3/4 | 0.065 | 4,090 (28) | 18,740 (129) | 4,310 (30) |
3/4 | 0.083 | 5,220 (36) | 20,310 (140) | 5,380 (37) |
1) Estimates only. Actual pressures should be calculated considering all stress factors in the system.
2) Based on calculations from API 5C3, using a wall tolerance of +/-10%
3) Based on ultimate strength burst calculations from API 5C3
4) Based on yield strength collapse calculations from API 5C3
Pw = reference working pressure rating for TP 316L at 100°F (38°C). To determine working pressure for grade/temperature combination, multiply Pw by adjustment factor.
Grade | 100°F (38°C) |
200°F (93°C) |
300°F (149°C) |
400°F (204°C) |
---|---|---|---|---|
TP 316L, seamless | 1.00 | 0.87 | 0.70 | 0.63 |
TP 316L, welded | 0.85 | 0.74 | 0.60 | 0.54 |
Alleima SAF 2205™, seamless | 2.17 | 2.00 | 1.77 | 1.60 |
Alleima SAF 2205™, welded | 1.84 | 1.70 | 1.50 | 1.36 |
Alloy 825, seamless | 1.33 | 1.17 | 1.10 | 1.03 |
Alloy 825, welded | 1.13 | 0.99 | 0.94 | 0.88 |
Alleima SAF 2507® , seamless | 2.67 | 2.33 | 2.17 | 1.70 |
Alleima SAF 2507® , welded | 2.27 | 1.98 | 1.84 | 1.45 |
1) Adjustment factors based on allowable stress in ASME.
Example: The maximum factors allowable working pressure for seamless 1/2 x 0.049 in. Alleima SAF 2507® tubing at 100°F (38°C) can be calculated as:
4,630 psi – Pressure rating for TP 316L at 100°F (38°C)
x 2.67 – Adjustment factor for Alleima SAF 2507, seamless at 100°F (38°C)
12,362 psi – Working pressure rating for Alleima SAF 2507® tubing
Pb = reference burst pressure for TP 316L at 100°F. To determine burst pressure for grade/temperature combination, multiply Pb by adjustment factor.
Grade | 100°F (38°C) |
200°F (93°C) |
300°F (149°C) |
400°F (204°C) |
---|---|---|---|---|
TP 316L, seamless | 1.00 | 0.93 | 0.87 | 0.80 |
TP 316L, welded | 0.85 | 0.79 | 0.74 | 0.68 |
Alleima SAF 2205™, seamless | 1.71 | 1.33 | 1.20 | 1.07 |
Alleima SAF 2205™, welded | 1.45 | 1.13 | 1.02 | 0.91 |
Alloy 825, seamless | 1.13 | 1.07 | 1.00 | 0.87 |
Alloy 825, welded | 0.96 | 0.91 | 0.85 | 0.74 |
Alleima SAF 2507® , seamless | 1.97 | 1.75 | 1.57 | 1.35 |
Alleima SAF 2507® , welded | 1.64 | 1.47 | 1.31 | 1.13 |
1) Adjustment factors based on ultimate strength in ASME.
Example: The maximum factors burst pressure for seamless 3/8 x 0.049 in. Alleima SAF 2507® tubing at 200°F (93°C) can be calculated as:
21,750 psi – burst pressure rating for TP 316L at 100°F (38°C)
x 1.73 – Adjustment factor for Alleima SAF 2507, seamless at 200°F (93°C)
37,627 psi – burst pressure rating for Alleima SAF 2507® tubing
Pc = reference collapse pressure rating for TP 316L at 100°F (38°C). To determine collapse pressure for grade/temperature combination, multiply Pc by adjustment factor.
Grade | 100°F (38°C) |
200°F (93°C) |
300°F (149°C) |
400°F (204°C) |
---|---|---|---|---|
TP 316L, seamless | 1.00 | 0.87 | 0.70 | 0.63 |
TP 316L, welded | 0.85 | 0.74 | 0.60 | 0.54 |
Alleima SAF 2205™, seamless | 2.17 | 2.00 | 1.77 | 1.60 |
Alleima SAF 2205™, welded | 1.84 | 1.70 | 1.50 | 1.36 |
Alloy 825, seamless | 1.33 | 1.17 | 1.10 | 1.03 |
Alloy 825, welded | 1.13 | 0.99 | 0.94 | 0.88 |
Alleima SAF 2507® , seamless | 2.67 | 2.33 | 2.17 | 1.70 |
Alleima SAF 2507® , welded | 2.27 | 1.98 | 1.84 | 1.45 |
1) Adjustment factors based on yield strength in ASME.
Example: The maximum factors collapse pressure for seamless 1/4 x 0.035 in. Alloy 825 tubing at 200°F (93°C) can be calculated as:
6,600 psi – Collapse pressure rating for ASTM 316L at 100°F (38°C)
x 1.17 – Adjustment factor for Alloy 825 seamless at 200°F (93°C)
7,722 psi – Collapse pressure rating for Alloy 825 tubing