Batch hardening deep freezing -70°C/-95°F of Sandvik 13C26 knife steel

Need to know more?

Call us Email us

Buy samples of Sandvik 14C28N knife steel

Now in stock, so don't miss this opportunity!

Current availability:

  • USA & Canada: Hobbyists / consumers over 18 years of age and business customers
  • European Union: Hobbyists / consumers over 18 years of age and business customers
  • Rest of the world: Business customers only

Buy sample


Temperature should be equalized at 850°C/1560°F for 30 minutes to avoid unnecessary temperature variations.

Austenitizing

Batch furnace. 30 minutes in furnace.

Quenching

Quench as rapidly as possible. For optimal results 600°C (1110°F) should be reached within 2 minutes or less.

Deep freezing

The material only needs to reach the desired deep freezing temperature, no soaking-time is required.

Tempering (2 hours)
HardnessTemperature
62 HRC 175°C (345°F)
60 HRC 225°C (435°F)
58 HRC 350°C (660°F)