Batch hardening of Sandvik 13C26 knife steel

Need to know more?

Call us Email us

Buy samples of Sandvik 14C28N knife steel

Now in stock, so don't miss this opportunity!

Current availability:

  • USA & Canada: Hobbyists / consumers over 18 years of age and business customers
  • European Union: Hobbyists / consumers over 18 years of age and business customers
  • Rest of the world: Business customers only

Buy sample


Austenitizing

Batch furnace. 30 minutes in furnace.

Quenching

Quench as rapidly as possible. For optimal results 600°C (1110°F) should be reached within 2 minutes or less.

Tempering (2 hours)
HardnessTemperature
59 HRC 175°C (345°F)
57 HRC 225°C (435°F)
54 HRC 350°C (660°F)