Piece hardening of Sandvik 14C28N knife steel

Need to know more?

Call us Email us

Austenitizing

Belt furnace. Time in furnace according to the table.

Thickness Thickness Time
mm in. minutes
2.5 0.100 5
3.0 0.118 6
3.25 0.128 7
3.5 0.138 8
3.75 0.148 10
4.0 0.157 12
4.9 0.192 25

Quench

Quench as rapidly as possible. For optimal results 600°C (1110°F) should be reached within 2 minutes or less.

Tempering , 2 hours
Hardness Temperature
59 HRC 175oC (345oF)
57 HRC 225oC (435oF)
55 HRC 350oC (660oF)