Sandvik 7RE10 is an austenitic, stainless chromium-nickel steel of the 25/20 type. It has good resistance to carburization, sulfidation and oxidation combined with moderate creep strength and structural stability. Maximum service temperature in air is 1100°C (2010°F).
Standards
-
ASTM: 310S, 310H -
UNS: S31008, S31009 -
EN Number: 1.4845 -
W.Nr.: 1.4845 -
DIN: X12 CrNi 25 21 -
SS: 2361 -
AFNOR: Z12CN25-20 -
BS: 310S31
Product standards
ASTM A-314
Suitable for production of flanges etc. acc. to ASTM A-182
Certificates
Status according to EN 10 204/3.1
Chemical composition (nominal) %
C |
Si | Mn | P |
S |
Cr | Ni | Mo | Others |
---|---|---|---|---|---|---|---|---|
0.05 | 0.5 | 1.3 | ≤0.030 | ≤0.010 | 24.5 | 21 | - | - |
Forms of supply
Sizes and tolerances
Round-cornered square, as well as round billets, are produced in a wide range of sizes according to the following tables. Larger sizes offered on request.
Surface conditions
Square billets
Unground, spot ground or fully ground condition.
Round billets
Peel turned or black condition.
Size | Tolerance | Length |
---|---|---|
mm | mm | m |
80 | +/-2 | 4 - 6.3 |
100, 114, 126, 140, 150 | +/-3 | 4 - 6.3 |
160, 180, 195, 200 | +/-4 | 4 - 6.3 |
>200 - 350 | +/-5 | 3 - 5.3 |
Sizes and tolerances apply to the rolled/forged condition.
Size | Tolerance | Length |
---|---|---|
mm | mm | m |
75 - 200 (5 mm interval) | +/-1 | max 10 |
>200 - 450 | +/-3 | 3 - 8 |
Size | Tolerance | Length |
---|---|---|
mm | mm | m |
77 - 112 (5 mm interval) | +/-2 | max 10 |
124, 134 | +/-2 | max 10 |
127, 147, 157 | +/-2 | max 10 |
142, 152, 163 | +/-2 | max 10 |
168, 178, 188 | +/-2 | max 10 |
183, 193 | +/-2 | max 10 |
Other products
- Hollow bar
Mechanical properties
At 20°C
Proof strength | Tensile strength | Elong. | Hardness | ||
---|---|---|---|---|---|
Rp0.2a | Rp1.0a | Rm | Ab | A2" | HRB |
MPa | MPa | MPa | % | % | |
≥220 | ≥240 | 515-750 | ≥35 | ≥35 | ≤90 |
At 68°F
Proof strength | Tensile strength | Elong. | Hardness | ||
---|---|---|---|---|---|
Rp0.2a | Rp1.0a | Rm | Ab | A2" | HRB |
ksi | ksi | ksi | % | % | |
≥32 | ≥35 | 75-109 | ≥35 | ≥35 | ≤90 |
1 MPa = 1 N/mm2
a) Rp0.2 and Rp1.0 correspond to 0.2% offset and 1.0% offset yield strength, respectively.
b) Based on L0 = 5.65 √S0 where L0 is the original gauge length and S0 the original cross-section area.
At high temperatures
Temperature
|
Proof strength
|
|
---|---|---|
Rp0.2 | Rp1.0 | |
°C | MPa | MPa |
min | min | |
50 | 200 | 230 |
100 | 190 | 220 |
150 | 180 | 210 |
200 | 170 | 200 |
250 | 165 | 195 |
300 | 160 | 190 |
350 | 155 | 185 |
400 | 150 | 180 |
450 | 145 | 175 |
500 | 140 | 170 |
550 | 135 | 165 |
600 | 130 | 160 |
650 | 125 | 155 |
700
|
120
|
150
|