Sanicro® 31HT, commonly known as Alloy 800HT, is an austenitic nickel-iron-chromium alloy. It is characterized by:
- High creep strength
- Very good resistance to oxidation
- Good resistance to combustion gases
- Very good resistance to carburization
- Good resistance to nitrogen absorption
- Good structural stability at high temperatures
- Good weldability
The grade can be used at temperatures up to about 1100°C (2010°F). In order to have the best ductility this grade should be used above 700°C (1290°F). Because of its high nickel content and prescribed maximization of (Ti + Al) content, Sanicro® 31HT shows extremely little tendency to precipitation of embrittling phases.
Standards
-
UNS: N08810/N08811 -
EN Number: 1.4959 -
W.Nr.: 1.4876/1.4959
Product Standards
Suitable for the production of flanges etc. according to ASTM B564
Chemical composition according to EN 10095.
Certificate
Status according to EN 10 204/3.1
Chemical composition (nominal) %
C | Si | Mn | P | S | Cr | Ni | Ti | Al | Fe |
---|---|---|---|---|---|---|---|---|---|
0.07 | 0.6 | 0.6 | ≤0.025 | ≤0.010 | 20.5 | 30 | 0.5 | 0.5 | bal. |
Applications
The combination of good hot strength, with good structural stability and ductility, makes Sanicro 31HT a suitable grade for various products in plants producing synthetic gas for ammonia, methanol and town gas. Sanicro 31HT is a good choice for applications involving long term exposure at high temperatures and corrosive environments.
Industrial categories | Typical applications |
---|---|
Chemical industry | Flanges |
Industrial heating | Valves |
Petrochemical industry | Fittings |
Pulp and paper industry | Couplings |
Oil & Gas industry | Rings |
Seals | |
Bolts and nuts | |
Shafts | |
Forgings | |
Discs | |
Pigtails and headers |
Corrosion resistance
Since Sanicro® 31HT is used for its high temperature strength, it is often exposed to high-temperature reactions, such as oxidation and carburization. Sanicro® 31HT is highly resistant to oxidation, both at constant and cyclically varied temperatures because of the high chromium and nickel contents. The service temperature in air should not exceed 1100°C (2010°F). The high nickel content also gives good resistance to carburizing environments, whilst the high chromium content provides good resistance to many sulphur-containing atmospheres at high temperatures.
Sanicro® 31 HT has roughly the same resistance as Alloy 800 to general corrosion and pitting. Due to the high nickel content, its resistance to stress corrosion is also good.
Owing to its relatively high carbon content and the heat treatment applied, Sanicro® 31HT displays a certain tendency to intergranular corrosion.
This problem can be disregarded where high temperature operations are concerned, but should be observed in cases where the alloy is exposed to corrosive condensates or pickling solutions. Sanicro® 31HT has passed the Strauss-test according to ASTM A262 Practice E.
For further information regarding corrosion resistance of Sanicro® 31HT, please see the data sheet for Seamless tube and pipe Sanicro® 31HT. The data should be considered in the knowledge that it may not be applicable for thick sections, such as forgings.
Forms of supply
Sizes and tolerances
Round-cornered square, as well as round billets, are produced in a wide range of sizes according to the following tables. Larger sizes offered on request.
Surface conditions
Square billets
Unground, spot ground or fully ground condition.
Round billets
Peel turned or black condition.
Size mm |
Tolerance mm |
Length m |
---|---|---|
80 | +/-2 | 4 - 6.3 |
100, 114, 126, 140, 150 | +/-3 | 4 - 6.3 |
160, 180, 195, 200 | +/-4 | 4 - 6.3 |
>200 - 350 | +/-5 | 3 - 5.3 |
Sizes and tolerances apply to the rolled/forged condition.
Size mm |
Tolerance mm |
Length m |
---|---|---|
75 - 200 (5 mm interval) | +/-1 | max 10 |
>200 - 450 | +/-3 | 3 - 8 |
Size mm |
Tolerance mm |
Length m |
---|---|---|
77 - 112 (5 mm interval) | +/-2 | max 10 |
124, 134 | +/-2 | max 10 |
127, 147, 157 | +/-2 | max 10 |
142, 152, 163 | +/-2 | max 10 |
168, 178, 188 | +/-2 | max 10 |
183, 193 | +/-2 | max 10 |
Other products
Seamless tube and pipe
Hollow bar
Heat treatment
Sanicro® 31HT is designed for high temperature service. For optimum creep rupture strength, the material should be solution annealed to obtain an average grain size of ASTM No 5 or coarser. The recommended temperature is 1150-1200°C (2100-2190°F). Soaking time depends on the product size and type of furnace. Rapid cooling in water is also recommended. Excessive grain growth should be avoided.
Mechanical properties
Sanicro® 31HT conforms to the required mechanical properties according to specification ASTM B564. Testing is performed on separately solution annealed and quenched test pieces.
At 20°C (68°F)
Proof strength
|
Tensile strength
|
Elongation
|
---|---|---|
Rp0.21)
|
Rm
|
A
|
MPa
|
MPa
|
%
|
≥172
|
≥448
|
≥30
|
At 68 oF
Proof strength
|
Tensile strength
|
Elongation
|
---|---|---|
Rp0.21)
|
Rm
|
A
|
ksi
|
ksi
|
%
|
≥25
|
≥65
|
≥30
|
1) Corresponds to 0.2 % offset yield strength
At high temperatures
Fig. 1 shows indicative values for tensile strength properties of Sanicro® 31HT at high temperatures.
Figure 1. Minimum high temperature tensile strength properties for Sanicro 31HT are based on datasheets seamless tube and pipe. Since the tubes have thin walls the values should only be used as indicative values for forgings. (Proof strength corresponds to 0.2% offset yield strength.)
Physical properties
Density: 7.9 g/cm3
Temperature, °C | J/kg °C | Temperature, °F | Btu/lb °F |
---|---|---|---|
20 | 470 | 68 | 0.11 |
200 | 520 | 400 | 0.12 |
400 | 570 | 800 | 0.14 |
600 | 605 | 1200 | 0.15 |
800 | 630 | 1600 | 0.15 |
1000 | 655 | 2000 | 0.16 |
1) Typical values
Temperature, °C | W/m °C | Temperature, °F | Btu/(ft h °F) |
---|---|---|---|
20 | 12 | 68 | 6.5 |
200 | 16 | 400 | 9 |
400 | 19 | 800 | 11.5 |
600 | 22 | 1200 | 13.5 |
800 | 25 | 1600 | 15 |
1000 | 28 | 2000 | 16.5 |
1) Typical values
Temperature, °C | Per °C | Temperature, °F | Per °F |
---|---|---|---|
30-200 | 16 | 86-400 | 9 |
30-400 | 16.5 | 86-800 | 9.5 |
30-600 | 17 | 86-1200 | 9.5 |
30-800 | 18 | 86-1600 | 10 |
30-1000 | 18.5 |
1) typical values (x10-6)
Temperature, °C | MPa | Temperature, °F | ksi |
---|---|---|---|
20 | 200 | 68 | 29.0 |
200 | 190 | 400 | 27.5 |
400 | 175 | 800 | 25.0 |
600 | 160 | 1200 | 22.5 |
800 | 145 | 1400 | 21.5 |
1000 | 130 | 1800 | 19.0 |
1) typical values (x103)
Hot working
The hot forming range for Sanicro® 31HT is 900-1200°C (1600-2200°F). To avoid chilling the metal during working, preheating tools and dies is recommended. Heavy forging should not be carried out so rapidly that the metal becomes overheated. Because of the risk of intermetallic precipitations in the temperature range 540-760°C (1000-1400°F), water cooling is recommended after hot working, in order to avoid intergranular corrosion.
Welding
The weldability of Sanicro® 31HT is good. Suitable methods of fusion welding are manual metal-arc welding (MMA/SMAW) and gas-shielded arc welding, with the TIG/GTAW method as first choice. Preheating and post-weld heat treatment are not necessary.
The welding of fully austenitic steels often entails the risk of hot cracking, particularly if the weldment is under constraint. To reduce the cracking risk, the welding should be carried out with a low heat input.
For Sanicro® 31HT, heat input of <1.0 kJ/mm and interpass temperature of <100°C (210°F) are recommended. A string bead welding technique should be used.
Recommended filler metals for temperature under 800 °C
TIG/GTAW or MIG/GMAW welding
ISO 18274 S Ni 6082/AWS A5.14 ERNiCr-3 (e.g. Exaton Ni72HP)
MMA/SMAW welding
ISO 14172 E Ni 6182/AWS A5.11 ENiCrFe-3 (e.g. Exaton Ni71)
Recommended filler metals for temperature ≥800 °C
TIG/GTAW or MIG/GMAW welding
ISO 18274 S Ni 6617/AWS A5.14 ERNiCrCoMo-1 (e.g. Exaton Ni53)
MMA/SMAW welding
ISO 14172 E Ni 6117/AWS A5.11 ENiCrCoMo-1
Machining
Machining Sanicro® 31HT, as with other stainless steels, requires an adjustment to tooling data and machining method, in order to achieve satisfactory results. Compared to Sanmac® 316/316L, the cutting speed must be reduced by approximately 45-55%, when turning Sanicro® 31HT with coated, cemented carbide tools. Much the same applies to other operations. Feeds should only be reduced slightly and with care.
Detailed recommendations for the choice of tools and cutting data are provided in the data sheet for Sanmac® 316/316L.