Sulphuric acid + chlorides

These corrosion data are mainly based on results of general corrosion laboratory tests, carried out with pure chemicals and water solutions nearly saturated with air (the corrosion rate can be quite different if the solution is free from oxygen).

All concentrations are given in weight-% and the solvent is water if nothing else is shown. The corrosion data apply to annealed materials with normal microstructure and clean surfaces, throughout.

Symbol clarification

Sulphuric acid + chlorides, (200 ppm CI-)
Conc.H2SO4% 1 1 1 1 5 5 5 10 10 10 10 10 20 20 20 20
Conc.Cl-ppm 200 200 200 200 200 200 200 200 200 200 200 200 200 200 200 200
Temp.°C 70 80 90 100 70 80 90 50 60 70 80 90 40 50 60 70
Grade or type of alloy:
Carbon steel
13 Cr
Sandvik 1802
Sandvik 3R12
Sandvik 3R60 0 1
18Cr13Ni3Mo 1)
17Cr14Ni4Mo 2)
Sandvik 2RK65 ('904L') 0 1 1 0 2 0 0 2 0 1
Sanicro 28 0 0 0 0 0 1 0 0 1 1
254 SMO 0 0 0 2 0 0 2 0 0 2 2 0 1
654 SMO 0
SAF 2304 2 2
SAF 2205 0 0 2 0 2 2 2
SAF 2507 0 0 0 0 0 0 0 2 0 0 0 0
SAF 2707 HD 0
SAF 2906 0
SAF 3207 HD 0
Ti

1) ASTM 317L, e.g. Sandvik 3R64
2) EN 1.4439, e.g. Sandvik 3R68

Sulphuric acid + chlorides
Conc.H2SO4% 20 20 30 30 30 30 40 40 40 50 50
Conc.Cl-ppm 200 200 200 200 200 200 200 200 200 200 200
Temp.°C 80 90 30 40 50 60 15 25 40 50 60
Grade or type of alloy:
Carbon steel
13 Cr
Sandvik 1802
Sandvik 3R12
Sandvik 3R60 2
18Cr13Ni3Mo 1)
17Cr14Ni4Mo 2)
Sandvik 2RK65 ('904L') 2 0 1 2 1 1
Sanicro 28 1 0 1 1 0 0 0 0 0
254 SMO 1 2 0 1 1 0 0 0
654 SMO
SAF 2304
SAF 2205 2 2 2 2 0
SAF 2507 2 2 2
SAF 2707 HD 2
SAF 2906 2
SAF 3207 HD 1
Titanium (CP Ti)

1) ASTM 317L, e.g. Sandvik 3R64
2) EN 1.4439, e.g. Sandvik 3R68

Sulphuric acid + chlorides
Conc.H2SO4% 1 1 1 1 3 3 5 5 5 5 5 5 10 10 10
Conc.Cl-ppm 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000
Temp.°C 70 80 90 100=BP 40 50 50 60 70 80 90 100 20 40 50
Grade or type of alloy:
Carbon steel
13 Cr
Sandvik 1802
Sandvik 3R12
Sandvik 3R60 0 1 0
18Cr13Ni3Mo 1)
17Cr14Ni4Mo 2)
Sandvik 2RK65 ('904L') 0 1 0 1 0 0 1
Sanicro 28 0 0 0 0 0 0 0 0 0
254 SMO 0 0 0 0 0 0 0 0 1
654 SMO 0 0 0 1 0 0 0 0 0 0 0 0
SAF 2304 0 0 1 2
SAF 2205 0 1
SAF 2507 1 0 0 0 0 0 0 0 2 0 0 0
SAF 2707 HD 0
SAF 2906 0
SAF 3207 HD 0
Titanium (CP Ti)

1) ASTM 317L, e.g. Sandvik 3R64
2) EN 1.4439, e.g. Sandvik 3R68

Sulphuric acid + chlorides
Conc.H2SO4% 10 10 10 15 15 20 20 20 20 30 30 30 30 40 40
Conc.Cl-ppm 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000
Temp.°C 60 70 80 50 60 20 30 40 50 15 30 40 50 15 30
Grade or type of alloy:
Carbon steel
13 Cr
Sandvik 1802
Sandvik 3R12
Sandvik 3R60
18Cr13Ni3Mo 1)
17Cr14Ni4Mo 2)
Sandvik 2RK65 ('904L') 0 1 1 1
Sanicro 28 0 0 1 0
254 SMO 0 0 1 1
654 SMO 0 0 0 0 0 0 0 0 0 0 0 0 2 0 1
SAF 2304 2 2
SAF 2205
SAF 2507 0 1 2 1 2 1 2
SAF 2707 HD 0 0
SAF 2906 0 0
SAF 3207 HD 0 0 0
Titanium (CP Ti)

1) ASTM 317L, e.g. Sandvik 3R64
2) EN 1.4439, e.g. Sandvik 3R68

Sulphuric acid + chlorides
Conc.H2SO4% 50 50 60 60 70 70 80 80 90 90 98 98
Conc.Cl-ppm 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000 2000
Temp.°C 15 30 15 30 15 30 15 30 15 30 15 30
Grade or type of alloy:
Carbon steel
13 Cr
Sandvik 1802
Sandvik 3R12
Sandvik 3R60
18Cr13Ni3Mo 1)
17Cr14Ni4Mo 2)
Sandvik 2RK65 ('904L') 1 0 0 0 0 1 1 0 0
Sanicro 28
254 SMO 1 1 0 1 0 1 1 1
654 SMO 1 1 1 1 0 1 0 0 2
SAF 2304
SAF 2205
SAF 2507
Titanium (CP Ti)

1) ASTM 317L, e.g. Sandvik 3R64
2) EN 1.4439, e.g. Sandvik 3R68

Symbol clarification

These corrosion tables use a number of symbols, having the following meanings:

SymbolDescription
0 Corrosion rate less than 0.1 mm/year. The material is corrosion proof.
1 Corrosion rate 0.1—1.0 mm/year. The material is not corrosion proof, but useful in certain cases.
2 Corrosion rate over 1.0 mm/year. Serious corrosion. The material is not usable.
p, P Risk (severe risk) of pitting and crevice corrosion.
c, C Risk (Severe risk) of crevice corrosion. Used when there is a risk of localised corrosion only if crevices are present. Under more severe conditions, when there is also a risk of pitting corrosion, the symbols p or P are used instead.
s, S Risk (Severe risk) of stress corrosion cracking.
ig Risk of intergranular corrosion.
BP Boiling solution.
ND No data. (Used only where there are no actual data to estimate the risk of localised corrosion instead of p or s).

Disclaimer: Laboratory tests are not strictly comparable with actual service conditions. Accordingly, Sandvik makes no warranties, express or implied, and accept no liability, compensatory or consequential, for the performance of different materials in individual applications that may be based on the information provided in this publication.