Den här sidan finns enbart på Engelska (This page is only available in English)

The hardening programs are carefully matched to the various Alleima steel grades. Choose the furnace type to suit either individual pieces or an entire batch. Then select a steel grade.

The hardening cycle starts with heating from room temperature to the required hardening temperature (A = austenitizing) of between 1050 and 1090°C (1922 and 1994°F), depending on the steel grade.

The material is then quenched (Q = quench) to 600°C in the space of less than 2 minutes, possibly followed by deep-freezing (DF = deep-freezing) to between –20 and -70°C (-4 and -94°F).

This is followed by the tempering process (T = tempering), during which the material is heated to 175 - 350°C (347 - 662°F), depending on the required hardness.

Belt furnace
Steel grade Piece
hardening
Piece hardening,
with deep freezing -20°C (-5°F)
Piece hardening,
with deep freezing -70°C (-95°F)
Alleima® 7C27Mo2
Alleima® 12C27M
Alleima® 12C27
Alleima® 13C26
Alleima® 14C28N
Alleima® 19C27
Alleima® 10C16Mo3V1 See datasheet
Alleima® 10C28Mo2 See datasheet
Batch furnace
Steel grade Batch
hardening
Batch hardening, with deep freezing -20°C (-5°F) Batch hardening,
with deep freezing -70°C (-95°F)
Alleima® 7C27Mo2
Alleima® 12C27M
Alleima® 12C27
Alleima® 13C26
Alleima® 14C28N
Alleima® 19C27