Selected cobalt alloys incl. chemical composition (nominal), %
Alloy (UNS) Description Co Fe C Cr Ni Mo Si Mn W V
CO212 - Bal. 0.75 0.02* 28.5 ≤1.0 6.0 ≤1.0 ≤1.0
-
-
CO502 Wear resistant alloy, hardness Rc 41-45. Bal. ≤3.0 2.0 29.0 ≤3.0
-
≤2.0 ≤1.0 8.5
-
CO90 - Bal. ≤3.0 0.1 20.0 10.0
-
≤0.4 1.5 15.0
-
Co49Fe2V Soft magnetic alloy Bal. 49.0 ≤0.05
-
-
-
≤1.0 ≤1.0
-
2.0

* A range of different carbon levels are available.

Other cobalt alloys are also available. Contact us to discuss Sandvik's full range of metal powder alloys.

Brazing alloys

Cobalt brazing alloys

Cobalt alloy suitable for use as filler metal for brazing applications.

Selected cobalt brazing alloys incl. chemical composition (nominal), %
Alloy EN 1044 Melting range, ºC Co Ni Cr Si Fe C P Other
HTN 12 CO 101 1120–1150* Bal. 17.0 10.0  8.0  1.0 ≤0.4 ≤0.02 W 0.4 

* Approximate values

Other cobalt brazing alloys are also available. Contact us to discuss Sandvik's full range of metal powder alloys.

Thermal spray alloys

Cobalt thermal spray alloys

The Osprey range of cobalt thermal spray alloys includes:

  • Self fluxing alloys
  • Non self fluxing alloys

Self fluxing cobalt alloys

Self fluxing cobalt alloy formulations giving a wide compositional variation that will produce coatings with optimum wear resistance. Alloy selection depends upon the application requirements, including wear resistance characteristics and the working environment. The metal powder is supplied to suit all thermal spraying and welding systems.

Selected self fluxing cobalt alloys incl. chemical composition (nominal), %
Alloy Hardness, Rc Co C Cr Si B Fe Ni W
Co 201 58–62 Bal. 1.5 19.0 3.0 - 3.0* 13.0 15.0
Co 441 42–47 Bal. 0.75 19.0 3.0 1.75 3.0* 13.0 8.0
Co 501 48–52 Bal. 1.0 19.0 3.0 2.0 3.0* 13.0 10.5
Co 551 50–55 Bal. 1.35 19.0 3.0 2.5 3.0* 13.0 13.0

* Maximum value

Non self fluxing cobalt alloys

Non self fluxing cobalt alloys formulated to produce high-integrity coatings using plasma and high-velocity thermal spray systems. The alloys are selected to give a wide range of wear resistance properties for abrasion, corrosion and erosion at elevated temperatures.

Alloy Hardness, Rc Co C Cr Ni Mo Fe Si W Mn
Selected non self fluxing cobalt alloys incl. chemical composition (nominal), %
Co 212 26–30 Bal. 0.25 27.0 1.0  6.0 2.0* 2.0* - ≤1.0
Co 222 26–30 Bal. 0.25 27.0 1.0  6.0  1.0* 2.0* - ≤1.0
Co 310 38–42 Bal. 0.5 25.0 10.0 - 1.5* 2.0* 7.0 ≤1.0
Co 400 51–58 Bal. 0.08 8.5 3.0  28.5 1.0* 2.6* - ≤1.0
Co 452 38–42 Bal. 1.0 29.0 3.0* - 3.0* 2.0* 5.0 ≤1.0
Co 502 41–45 Bal. 1.5 29.0 3.0* - 3.0* 2.0* 8.0 ≤1.0
Co 552 50–54 Bal. 2.5 30.0 3.0* - 3.0* 2.0* 13.0 ≤1.0
Co 800 54–62 Bal. 0.08 17.5 3.0 28.5 1.0* 3.4* - ≤1.0
Co F01  40–44 Bal. 1.5 25.0 22.0 - 1.0* 2.0* 12.0 ≤1.0

* Maximum value