Sandvik 13C26 is a martensitic stainless chromium steel supplied in strip form. The grade is mainly supplied in annealed or cold rolled condition, characterized by:
- Soft delivery condition
- Good formability
- Good blanking properties
After heat treatment, Sandvik 13C26 is characterized by:
- High hardness
- Good corrosion resistance
- High wear resistance
Standards
-
: X65Cr13
Product standards
ISO 7153-1
Chemical composition (nominal)
C | Si | Mn | P | S | Cr |
---|---|---|---|---|---|
0.68 | 0.4 | 0.7 | ≤0.025 | ≤0.010 | 13 |
Applications
Sandvik 13C26 is mainly used for ophthalmologic and surgical surgical blades. It is also a standard grade for razor blades and used for different types of knives.
Forms of supply
The strip can be supplied either in coils or as straightened lengths of 0.5 - 4.0 meter (1.6 - 13.1 feet). The coil weight is max 5 kg/mm (280 lb/in.) of strip width.
Hardening and tempering of the strip steel is required to achieve the correct finish and to meet the properties necessary for the end user.
Thickness | Width | ||
---|---|---|---|
mm (in.) | mm (in.) | ||
min. | max. | min. | max. |
0.1 (0.0039) | 1.0 (0.039) | 5 (0.197) | 350 (13.78) |
Other sizes can be supplied to meet specific requirements.
Tolerances
The thickness and width tolerances are +/- tolerances to the nominal size. The normal tolerance classes for most of our strip products are T2 and B1. Tighter tolerances as well as other tolerance limits can be offered upon request.
Heat treatment
Hardening data and Tempering data: Piece hardening
Austenitizing
Belt furnace. Time in furnace according to table
Thickness | Thickness | Time |
---|---|---|
mm | in. | minutes |
2.5 | 0.100 | 5 |
3.0 | 0.118 | 6 |
3.25 | 0.128 | 7 |
3.5 | 0.138 | 8 |
3.45 | 0.148 | 10 |
4 | 0.157 | 12 |
Quench
As rapid as possible, for optimal result 600°C (1110°F) should be reached within 2 minutes or less.
Hardness | Temperature |
---|---|
HRC | °C (°F) |
59 | 175 (345) |
57 | 225 (435) |
55 | 350 (660) |
Hardening data and Tempering data : Batch hardening
Temperature should be equalized at 850°C (1560°F) for 30 minutes to avoid unnecessary temperature variations.
Austenitizing
Batch furnace. 30 minutes in furnace.
Quench
As rapid as possible, for optimal result 600°C (1110°F) should be reached within 2 minutes or less.
Hardness | Temperature |
---|---|
HRC | °C (°F) |
59 | 175 (345) |
57 | 225 (435) |
55 | 350 (660) |
Hardness versus tempering temperature
Brittleness occurs with tempering above 450°C (840°F).
Mechanical properties
As delivered | Tensile strength Rm | Hardness | |
---|---|---|---|
MPa (ksi) | HV | HRC | |
Annealed | max. 800(116) | max. 250 | max. 22 |
Cold rolled | 830-1050 (121-152) | 260-328 | 24-33 |
Hardened and tempered | 1700-2000 (247-290) | 545-633 | 52-57 |
Mechanical properties can vary depending on the tempering parameters
Physical properties
The physical properties of a steel are related to a number of factors, including alloying elements, heat treatment and manufacturing route, but the data presented below can generally be used for rough calculations.
Density : 7.7 g/cm3 (0.28 lb/in.3)