SAF 2906™ is a high-alloy duplex (austenitic-ferritic) stainless steel with excellent corrosion resistance in caustic environments and environments with chlorides. SAF 2906™ characteristics:
- Excellent resistance to caustic environments, also in the presence of contaminants such as chlorides
- Excellent resistance to intergranular corrosion
- Excellent resistance to pitting and crevice corrosion
- High resistance to stress corrosion cracking (SCC)
- Good weldability
- Very high strength. The proof strength is about three times as high as for conventional austenitic stainless steels.
Standards
-
: S32906 -
: 1.4477
Product standards
- Seamless tube and pipe: ASTM A789, A790
- Bar steel: ASTM A479
- Plate: ASTM A240
Approvals
- Approved by the American Society of Mechanical Engineers (ASME) for use in accordance with ASME Boiler and Pressure Vessel Code, Section VIII, div. 1 and 2.
- PED (Pressure Equipment Directive) PED 2014/68/EU and AD2000 Merkblatt W2: Particular Material Appraisal (PMA), Austenitic-ferritic steel Sandvik SAF 2906.
Chemical composition (nominal)
C | Si | Mn | P | S | Cr | Ni | Mo | Cu | N |
---|---|---|---|---|---|---|---|---|---|
≤0.030 | 0.3 | 1.0 | ≤0.030 | ≤0.015 | 29 | 7 | 2.3 | ≤0.80 | 0.35 |
Applications
Typical applications for SAF 2906™ are:
- Caustic soda production: the material is suitable for use in piping systems from the cells up to the evaporation plant. It is also an excellent choice for very aggressive conditions, such as the evaporator tubes, in both diaphragm and membrane process.
- Alumina production: heat exchanger tubes and piping in the digestion of alumina
- Environments where high resistance to pitting and crevice corrosion is required
Corrosion resistance
Caustic environment
SAF 2906™ has, owing to its high chromium content, a very good resistance in caustic environments. For pure caustic soda, the performance of SAF 2906™ can be observed in the iso-corrosion diagram (0.1 mm/year), see Figure 1. In the production of caustic soda, however, impurities in the form of chlorides and chlorates are present. Usually, in the caustic soda manufacturing process Ni200 or high nickel alloys are used, especially in critical equipment such as the evaporators.
Results of corrosion tests in sodium hydroxide (NaOH) containing different amounts of sodium chloride (NaCl) and sodium chlorate (NaClO3 ), similar to the content found in the evaporation plants of diaphragm and membrane processes, are presented in Table 1, 2 and Figure 2. The results clearly indicate the good performance of SAF 2906™ in caustic environments.
Grade | Environment | Temperature, °C (°F) | Corrosion rate mm/year |
---|---|---|---|
SAF 2906 | 10% NaOH, 2% NaCl, 800 ppm ClO3- | 100 (212) | < 0.01 |
Boiling | < 0.01 | ||
50% NaOH, 7% NaCl, 800 ppm ClO3- | 100 (212) | < 0.01 | |
Boiling | 0.016 | ||
Sanicro 28 | 10% NaOH, 2% NaCl, 800 ppm ClO3- | 100 (212) | < 0.01 |
Boiling | < 0.01 | ||
50% NaOH, 7% NaCl, 800 ppm ClO3- | 100 (212) | < 0.01 | |
Boiling | 0.34 | ||
Ni200 | 10% NaOH, 2% NaCl, 800 ppm ClO3- |
100 (212) | < 0.01 |
Boiling | < 0.01 | ||
50% NaOH, 7% NaCl, 800 ppm ClO3- | 100 (212) | < 0.01 | |
Boiling | 0.15 |
Grade | Environment | Temperature | Corrosion rate mm/year |
---|---|---|---|
SAF 2906 | 32%NaOH + 30 ppm Cl- + 20 ppm NaClO3 | Boiling | < 0.01 |
50%NaOH + 30 ppm Cl- + 20 ppm NaClO3 | Boiling | < 0.01 | |
Ni200 | 32%NaOH + 30 ppm Cl- + 20 ppm NaClO3 | Boiling | < 0.01 |
50%NaOH + 30 ppm Cl- + 20 ppm NaClO3 | Boiling | < 0.01 |
Figure 1. Iso- corrosion diagram for SAF 2906 in pure NaOH, naturally aerated solution.
Figure 2. Corrosion rates in a mixture of 50% NaOH, 7% NaCl, 800 ppm ClO3-, boiling solution.
Pitting and crevice corrosion
SAF 2906™ has a carefully balanced composition with a high content of chromium and nitrogen and a moderate amount of molybdenum. This gives the material a high resistance to localized corrosion caused by chlorides. An index for comparing pitting corrosion resistance is the PRE number (Pitting Resistance Equivalent).
The PRE is defined as, in weight-PRE = %Cr + 3.3 x %Mo + 16 x %N
A very severe test for pitting or crevice corrosion is the ASTM G48 test, i.e. immersion in 6% FeCl3. Results for pitting test according to modified method A, as well as crevice corrosion testing according to method B, are presented in Table 3. The crevice corrosion test was performed with a crevice specified in the MTI-2 procedure, where an artificial crevice is mounted on the sample with a torque of 0.28 Nm. The critical pitting temperature (CPT) and the critical crevice temperature (CCT) are the temperatures where pitting or crevice corrosion starts to develop on the material.
Grade | PRE (min.) | CPT, °C (°F) | CCT, °C (°F) |
---|---|---|---|
SAF 2906 | 41.5 | 75 (167) | 42.5 (109) |
SAF 2507 | 42.5 | 80 (176) | 50 (122) |
SAF 2205 | 35 | 30 (86) | 18 (64) |
ASTM 316L | 26 | <10 (50) | <10 (50) |
Potentiostatic tests in solutions with different chloride contents are reported in Figure 3. Figure 4 shows the effect of increased acidity. In both cases the applied high potential, 600 mV SCE, corresponds to very harsh conditions, thus resulting in conservative data with a lower critical temperature compared with most practical situations.
Figure 3. Critical pitting temperature (CPT) at varying concentrations of sodium chloride, from 3 to 25% (potentiostatic determination at +600 mV SCE with surface ground to 600 grit paper).
Figure 4. Critical pitting temperature (CPT) in 3% NaCl with varying pH (potentiostatic determination at +600 mV SCE with surface ground to 600 grit paper).
Stress corrosion cracking (SCC)
SAF 2906™ has excellent resistance to chloride induced stress corrosion cracking (SCC). The resistance of various alloys to stress corrosion cracking (SCC) determined by constant load testing in aerated 40% CaCl2 , pH 1.5, at 100°C (210°F), (modified ASTM G36 method) is shown in Figure 5.
Figure 5. Constant load testing of SAF 2906™ and some other alloys in 40% CaCl2 , pH 1.5, at 100°C (212°F). Time to failure vs. applied stress in percentage of tensile strength is shown. Filled symbol: cracking, unfilled symbol: no cracking.
Nitric acid
Due to its balance of chromium and molybdenum, SAF 2906™ presents good resistance to nitric acid. The iso- corrosion diagram, see Figure 6, shows the performance of the material compared to Sandvik 2RE10, a high purity austenitic grade widely used for nitric acid.
Figure 6. Iso- corrosion diagram for SAF 2906™ and Sandvik 2RE10 in a naturally aerated, stagnant solution of nitric acid. The curves represent a corrosion rate of 0.1 mm/year.
Fabrication
Bending
The force needed for bending SAF 2906™ is higher than that for standard austenitic stainless steels which is a natural consequence of the higher yield strength.
Expanding
Compared with austenitic stainless steels, SAF 2906™ has a higher proof and tensile strength. This must be kept in mind when expanding tubes into tubesheets. Normal methods can be used, but the expansion requires higher initial force and should be undertaken in a one step operation. As a general rule, tube to tubesheet joints should be welded to ensure a leak free joint.
Machining
Being a dual phase material (austenitic-ferritic) SAF 2906™ will present a different wear picture from that of a single phase material like Sandvik 2RE69. The cutting speed must therefore be lower than that recommended for austenitic grades. Further information is available on request.
Forms of supply
Seamless tube and pipe
SAF 2906™ can be supplied as seamless tube and pipe. Tubes can be supplied straight or U-bent.
Other forms of supply:
- Fittings and flanges
- Plate, sheet and strip
- Bar steel
- Forged products
Heat treatment
The tubes are normally delivered in the heat treated condition. If additional heat treatment is needed after further processing, the following is recommended.
Solution annealing
1040-1080°C (1900-1980°F), rapid cooling in air or water.
Mechanical properties
The following figures apply to material in the solution annealed condition. If SAF 2906™ is exposed for prolonged periods to temperature ranges exceeding 280°C (540°F), the microstructure changes, which results in a reduction in toughness. This does not necessarily affect the behavior of the material at the operating temperature. The listed values are guaranteed for tube and pipe.
At 20°C (68°F)
Wall thickness | Proof strength | Tensile strength | Elong. | ||
---|---|---|---|---|---|
Rp0.2a) | Rm | Ab) | |||
mm | MPa | ksi | MPa | ksi | % |
min | min. | min. | min. | min. | |
<10 | 650 | 94 | 800 | 116 | 25 |
≥10 | 550 | 80 | 750 | 109 | 25 |
1 MPa = 1 N/mm2
a) Rp0.2 corresponds to 0.2% offset offset yield strength.
b) Based on L0 = 5.65 √S0 where L0 is the original gauge length and S0 the original cross-section area.
At high temperatures
Temperature | Wall thickness | Proof strength | Tensile strength, | Elong |
---|---|---|---|---|
Rp0.2 | Rm | A | ||
°C | mm | MPa | MPa | % |
min. | min. | min | ||
100 | <10 | 550 | 750 | 25 |
≥10 | 500 | 730 | 25 | |
200 | <10 | 470 | 720 | 25 |
≥10 | 430 | 700 | 25 | |
300 | <10 | 450 | 710 | 25 |
≥10 | 410 | 690 | 25 |
Temperature | Wall thickness | Proof strength | Tensile strength | Elong |
---|---|---|---|---|
Rp0.2 | Rm | A | ||
°F | in. | ksi | ksi | % |
min. | min. | min. | ||
200 | <0.4 | 80 | 109 | 25 |
≥0.4 | 73 | 106 | 25 | |
400 | <0.4 | 68 | 104 | 25 |
≥0.4 | 62 | 101 | 25 | |
600 | <0.4 | 65 | 103 | 25 |
≥0.4 | 59 | 100 | 25 |
Temperature
|
Stress
|
||||
---|---|---|---|---|---|
Tube wall thickness <10 mm
|
Tube wall thickness >10 mm
|
||||
oF | oC | ksi | MPa | ksi | MPa |
100 | 38 | 33.1 | 228 | 31.1 | 214 |
200 | 93 | 33.1 | 228 | 31.1 | 214 |
300 | 149 | 31.5 | 217 | 29.6 | 204 |
400 | 204 | 30.6 | 210 | 28.7 | 197 |
500 | 260 | 30.1 | 207 | 28.3 | 195 |
600 | 316 | 30.1 | 207 | 28.3 | 195 |
Impact strength
SAF 2906™ possesses a good impact strength. The ductility to brittle transition temperature is approximately -100°C (-150°F). Figure 7 shows the typical impact energy for SAF 2906™.
Figure 7. Typical impact energy curve for SAF 2906™ using half size (5 x 10 mm) Charpy V specimens (average of 3 at each temperature).
Physical properties
Density: 7.7 g/cm3, 0.28 lb/in3
Thermal conductivity
Temperature, °C | W/m °C | Temperature, °F | Btu/ft h°F |
---|---|---|---|
20 | 13 | 68 | 7 |
100 | 14 | 200 | 8 |
200 | 16 | 400 | 9 |
300 | 18 | 600 | 10 |
400 | 19 | 800 | 11 |
Specific heat capacity
Temperature, °C | J/kg °C | Temperature, °F | Btu/ft h°F |
---|---|---|---|
20 | 470 | 68 | 0.11 |
100 | 500 | 200 | 0.12 |
200 | 530 | 400 | 0.13 |
300 | 560 | 600 | 0.14 |
400 | 600 | 800 | 0.14 |
Thermal expansion
Mean values in temperature ranges (x10-6) SAF 2906™ has a coefficient of thermal expansion close to that of carbon steel. This gives SAF 2906™ definite design advantages over austenitic stainless steels. The values given in the table are average values in the temperature ranges.
Metric units, x10-6/°C
Temperature, °C | 30-100 | 30-200 | 30-300 | 30-400 |
---|---|---|---|---|
SAF 2906 | 11.5 | 12.0 | 12.5 | 12.5 |
Carbon steel | 12.5 | 13.0 | 13.5 | 14.0 |
ASTM 316L
|
16.5 | 17.0 | 17.5 | 18.0 |
Imperial units, x10-6/°F
Temperature, °F | 86-200 | 86-400 | 86-600 | 86-800 |
---|---|---|---|---|
SAF 2906 | 6.5 | 7.0 | 7.0 | 7.0 |
Carbon steel | 7.0 | 7.0 | 7.5 | 8.0 |
ASTM 316L
|
9.5 | 9.5 | 10.0 | 10.0 |
Resistivity
Temperature, °C | μΩm | Temperature, °F | μΩinch |
---|---|---|---|
20 | 0.81 | 68 | 31.9 |
Modulus of elasticity, x103
Temperature, °C | MPa | Temperature, °F |
ksi |
---|---|---|---|
20 | 200 | 68 | 29.0 |
100 | 194 | 200 | 28.2 |
200 | 186 | 400 | 26.9 |
300 | 180 | 600 | 26.0 |
Welding
The weldability of SAF 2906™ is good. Welding must be carried out without preheating and subsequent heat treatment is normally not necessary. Suitable method of fusion welding is gas tungsten arc welding GTAW/TIG with shielding gas of Ar+2% N2. For tube to tubesheet welding, it is recommended to use Ar+3% N2 as shielding gas to have proper weld metal structure.
For SAF 2906™, heat input of 0.2-1.5 kJ/mm and interpass temperature of <150°C (300°F) are recommended.
Recommended filler metals
GTAW/TIG welding
Exaton 29.8.2.L wire or strip electrodes are recommended for overlay welding of tubesheets and high-pressure vessels in cases where corrosion resistance, equal to that of SAF 2906™, is required.