Alleima_13C26_batch_hardening.png

Austenitizing

Batch furnace. 30 minutes in furnace.

Quenching

Quench as rapidly as possible. For optimal results 600°C (1110°F) should be reached within 2 minutes or less.

Tempering (2 hours)
Hardness Temperature
59 HRC 175°C (345°F)
57 HRC 225°C (435°F)
54 HRC 350°C (660°F)